ALUMINUM ALLOY 6061-T651




Typical Analysis in Weight Percent:

 

              Si                         0.4 - 0.8                             Mn                       0.15

              Fe                        0.7                                      Mg                       0.8 - 1.2

              Cu                        0.15 - 0.4                           Cr                        0.04 - 0.35

              Zn                        0.25                                    Ti                         0.15

              Other                   0.15



Typical Physical Properties:


Density: .098 lbs/in3 (2.71 g/cc)


Average Coefficient of Thermal Expansion (68 - 212 oF): 13.1 x 10-6/ oF


Melting Range (Approximate): 1080 - 1205 oF


Temper: T651 - Stress relieved by stretching.


Thermal Conductivity (at 77 oF): 1160 btu/in ft2 hr oF


Electrical Conductivity (at 68 oF, % of Int’l Annealed Copper Standard):

              Equal Volume:   43

              Equal Weight:    142


Electrical Resistivity (at 68 oF): 24 ohms-cir mil/foot



Typical Mechanical Properties:


Tensile Strength:

              Ultimate:            45 ksi

              Yield:                  40 ksi


Elongation (% in 2"):

              1/16" thick specimen:      12

              1/2" thick specimen:        17


Brinell Hardness (500 kg load - 10mm ball): 95


Ultimate Shearing Strength: 30 ksi


Endurance Limit: 14 ksi